Analysis and Treatment of fire tube leakage in sulfur acid waste heat boiler (Part 1)

1. Leakage location

1.1 Tube plate leakage

In the production operation, the leakage of waste heat fire-tube boiler often occurs at the position where the weld of the tube plate of the front smoke box fails. The waste heat fire-tube boiler is composed of a cylinder and a tube plate, and the tube plate and the fire tube are welded. In addition to the design pressure load [1], the welding position of the tubesheet is also subjected to the temperature load with obvious difference between the high temperature smoke of the front smoke box (about 1100℃) and the saturated water temperature in the drum (about 250℃). Therefore, the welding seam of the tubesheet and the fire tube is subjected to stress changes under both pressure and temperature conditions, and the maximum stress is generated at this position. When there is corrosion in the welding of tubesheet during operation, it will cause weld failure and leakage.

1.2 Fire tube leakage

The 1100℃ high temperature flue gas of the self-immolating sulfur furnace enters the smoke pipe of the lower pot shell, and after heat exchange with the water in the pot shell, the flue gas cools to 380℃, and then enters the conversion section of the sulfur acid making system. The water vapor mixture in the pot shell returns to the upper drum through the rising pipe, and then output saturated steam after separation in the drum.

If the boiler feed water and pot water do not meet the requirements of GB/T 12145(steam quality of thermal generating units and steam power equipment), It will cause a large number of silicon-containing compounds to enter the drum, and colloidal silicon will decompose into active silicon in the environment of high temperature, high pressure and high pH value, which will increase the content of active silicon in the pot water, and form adhesive scale and deposit on the drum, down tube, shell wall and fire tube [2]. Since the fire tube behind the front smoke box tube plate has the largest temperature difference, if the furnace water does not meet the requirements, a large amount of scale will accumulate in the fire tube behind the ceramic insulation tube behind the front smoke box tube plate. With the accumulation of scale, the heat transfer efficiency of the fire tube at this position will decrease. The material of the fire tube is 20G, allowing the metal wall temperature to be 430℃. The temperature of the metal wall is 280℃, and the temperature difference between the metal wall and the pot water is about 30℃. However, when the scale in the pot and the smoke pipe is accumulated, the heat transfer is seriously affected. When the scale is 1mm, the temperature difference reaches about 200℃; when the scale is 3mm, the temperature of the metal wall rises to 580℃, far exceeding the allowable use temperature of the material. The fire tube will bulge, deform or even crack under internal pressure at any time, resulting in fire tube leakage [2].

2. Leakage phenomenon

1. The boiler leakage will increase the boiler water supply and reduce the operating pressure.

2. Boiler leakage (under the condition that the heat secondary valve is open at the same degree) will lead to a lower temperature of the inlet furnace.

3. The leakage of water vapor from the boiler into the converter will absorb SO3 and cause the temperature to rise, and the temperature change in each section is abnormal, which is difficult to control, and in the process of gradually decreasing the temperature in the first section, the reaction will gradually move back to the second and third sections, resulting in high temperature in the second and third sections.

4. The leakage of boiler, economizer and high temperature superheater leads to the high temperature inlet flue gas temperature of the high temperature absorber.

5. The occurrence of a large number of leaks in the boiler and economizer will lead to a significant reduction in the dry acid absorption concentration (or a significant reduction in the amount of water added), and the bottom air chamber of the heat exchanger will produce more condensed acid.

6. Boiler leakage will lead to a significant increase in the water content of the inlet gas of the first stage of the converter [3].

3. Cause

1. In the process of repeatedly opening and stopping the device, thermal expansion and cold contraction occur, which makes the refractory material and thermal insulation steel pipe on the front tube plate fall off, and directly exposes the tube plate to high temperature flue gas, and is affected by condensing acid fog, resulting in sulfuric acid stress corrosion. Since this position is the weakest point of the boiler, stress concentration occurs and internal pressure is subjected to, resulting in tube plate weld failure and leakage.

2. Liquid sulfur is atomized from the sulfer gun into the sulfur burning furnace for combustion. If the atomization effect is not good, unburned sulfur vapor will be generated, and vulcanization corrosion will occur on the fire tube [4]. Sublimed sulfur and the fire tube produce iron sulfide under high temperature environment, and the pipe wall will be worn and thinned due to the long-term erosion of flue gas, and the outer wall of the fire tube will be subjected to boiler pressure, resulting in the fire tube internal concave damage and cracking and leakage.

3. During operation, in order to ensure the standard of phosphoric acid in the pan water, the dosage is greatly increased, and there are too many suspended substances and dissolved salts in the pan water, the surface viscosity of the pan water becomes larger, the resistance of bubbles rising increases, and a large number of tiny bubbles are stuck on the interface of soda water, resulting in “ Steam plug ” Resulting in overheating of the shell and the upper part of the tube plate, uneven heating of the tube plate, local overheating, resulting in a sudden increase in thermal stress, making the tube plate in front of the shell unstable deformation.

References

[1] YU Rui. Stress Analysis and Strength Check of hot pot boiler in 1800Kt/a sulfur acid making Unit [J]. Sulfuric Acid Industry, 2012 (03):43-47.

[2] Wen Zengyu. Analysis of tube plate leakage of sulfur-acid waste heat boiler [J]. Industrial Boiler, 2021 (04):47-51. (in Chinese)

[3] Zhang Weihong. Analysis and judgment of waste heat boiler leakage in sulfur acid production [J]. Sulfur and Phosphorus Design and Powder Engineering, 2015 (05):46-48. (in Chinese)

[4] Xie Jiankang. Analysis of pipe explosion causes and preventive measures of sulfur acid waste heat boiler [J]. Sulfur and Phosphorus Design and Powder Engineering, 2022 (06):30-34. (in Chinese)

主站蜘蛛池模板: 色综合色欲色综合色综合色综合r | 日韩欧洲亚洲 | 香蕉国产在线视频 | 国产精品com | 久久香视频| jjzz日本女人| 亚洲国产成人av在线电影播放 | 亚洲三级黄 | 影音先锋人妻啪啪av资源网站 | 国产免费视频青女在线观看 | 五月综合久久 | 少妇天天爽视频在线看网站 | 久久婷婷五月综合尤物色国产 | 国产精品青草久久久久婷婷 | 国产后进极品圆润翘臀在后面玩 | 国产精品夜夜夜爽阿娇 | 国内精品久久久久影院嫩草 | 天堂网av手机版 | 我要看免费黄色片 | 亚洲综合久久av一区二区三区 | 亚洲精品一区二区三区蜜桃久 | 狠狠色噜噜狠狠狠狠2022 | 十八禁视频在线观看免费无码无遮挡骂过 | 伊人91在线| 亚洲精品久久夜色撩人男男小说 | 狠狠躁夜夜躁人人爽天天bl | 国产美女精品自在线拍免费 | 人妻有码中文字幕在线 | www.夜夜骑 | 久久久久久国产精品免费无码 | 亚洲国产精品大学美女久久久爽 | 色婷婷在线视频 | 国产美女遭强高潮开双腿 | 在线观看一区二区三区国产免费 | 午夜大片免费男女爽爽影院 | 亚洲国产综合精品中文第一 | 久久久精品日韩免费观看 | 亚洲中文字幕人成影院 | 夜夜嗨av一区二区三区四季av | 18视频在线观看男男 | 成人片免费看 | 一级大片儿 | 国产女主播视频一区二区三区 | 免费观看啪啪黄的网站 | 51国偷自产一区二区三区的 | 日韩三级中文字幕 | 免费的又色又爽又黄的片捆绑美女 | 成人激情站 | 亚洲日产精品一二三四区 | 按摩害羞主妇中文字幕 | 盗摄中年夫妇啪啪免费观看 | 久久瑟瑟| 任我爽橹在线视频精品583 | 亚洲大乳高潮日本专区 | 伊人久久香 | 免费裸体美女网站 | www.夜夜骑 | 激烈娇喘叫1v1高h糙汉 | 国产超碰人人做人人爽aⅴ 91av中文字幕 | 波多野结av衣东京热无码专区 | 色婷婷久久久亚洲一区二区三区 | 人人干97| 男人让女人爽的免费视频 | 俄罗斯小14粉嫩呦萝 | 偷窥四川少妇野外啪啪 | 国产精品久久久免费 | 国产成人小视频 | 日韩伦人妻无码 | 午夜爽爽久久久毛片 | 丰满熟妇人妻av无码区 | 51久久精品夜色国产麻豆 | 亚洲aaaa级特黄毛片 | 热久久这里只有精品 | 一区二区三区日韩欧美 | 亚洲精品一二三区久久伦理中文 | 天天摸天天草 | 92午夜少妇极品福利无码电影 | 日本69视频 | 人成午夜大片免费视频77777 | 四虎久久久| 国产精品毛片大码女人 | 亚洲 综合 校园 欧美 制服 | www久久网 | 亚洲综合在线五月 | 国产成人精品免高潮在线观看 | 国产精品久久久一区二区 | 国产精品无码久久av不卡 | 国产精品一区二区三区四区五区 | 久久靖品 | 香港日本韩国三级网站 | 国产欧美va欧美va在线 | 日韩中文字幕免费在线观看 | 亚洲欧美在线观看 | 性一交一乱一伦一色一情孩交 | 久久久青草青草免费看 | 女人被男人桶30分钟无遮挡动态图 | 少妇情欲一区二区影视 | 亚洲成人网在线 | 日本一区二区不卡在线 |